How to Heat Treat AEB-L
Heat Treat Instructions for AEB-L Stainless Steel:
There are 2 versions, the first one is without Cryo treatment;
- Heat to 1560 F(849 C) and let come to temperature for 5 mins
- Ramp up to 1940 F (1060 C) and hold for 15 minutes
- Quench in oil, between plates or even air cool
- Temper at 300 F (149 C) for 60 HRC, 200 C for 58 HRC.
- Temper time not listed but assuming a solid 2 hours x 2 cannot hurt
The above is from Alpha Knife Supply in the US, we have just converted the Fahrenheit to Celcius.
The more advanced heat treat recipe including Cryo for higher HRC:
- Heat to 1560 F(849 C) and let come to temperature for 5 mins
- Heat to 1975 F (1079 C) and hold for 15 minutes
- Quench in oil, between plates or even air cool
- Cryo: Cool to -95 F (-70 C) with no hold time, just cool down and move to tempering
- Temper at 300 F (149 C) for 62 HRC, 400 F (200 C) for 60 HRC.
- Temper time not listed but assuming a solid 2 hours x 2 cannot hurt
30th Apr 2020
Recent Posts
-
WINNERS: 2024 Destruction Challenge
What a Destruction Challenge we had this year!! Here are the summary slides from the Winner ann …1st Nov 2024 -
Build Article: Damascus CuMai Knife
Build article on the Damascus Core Cu Mai Knife: SteelHeat treatmentGrindEtchingHandle shapingSheat …29th Oct 2024 -
Winner Announcements Live Stream: 30th Oct 2024 8 PM on Youtube
Join Jamie SausageMan Bishop for the Winner Announcements!When: Wed 30th October 2024Time: 8 PM DST …25th Oct 2024